The problem that Nimia from Mujeres Solares presented us with is that the paint used on the exterior of the solar oven (and the black plate in the bottom) flakes and peels off very easily. This is mainly an aesthetic problem. As such, one could very well ask the question, "Why do we care?" The answer is that Mujeres Solares is trying to market these ovens, and have in fact sold a large number of them. If the ovens look nice, they will sell better, meaning more people will buy them and cook with them instead of using wood. In addition, the profits generated will allow Mujeres Solares to give more ovens to their members and fund new programs to help people in Sabana Grande.
In order to solve this problem, we first tried to replicate the conditions under which the paint peeled. After some communication and inference, we concluded that the metal Mujeres Solares is trying to paint is galvanized (zinc electroplated) sheet metal, similar to the metal commonly used for ductwork in the United States. We were able to obtain some of that material. Next, we tried to obtain the paint Mujeres Solares uses. They used Corona brand "dura" oil paint. After extensive telephone and e-mail communication with the various departments of that paint company. we concluded we could not realistically get the paint here before the end of the semester. So, we ended up using a similar brand of oil paint to do our testing.
We used a test modeled after an ASTM standard for adhesion (test D 3359-02). We applied various pretreatments to the metal prior to painting in order to test their effectiveness relative to each other and control (no pretreatment). For the sand pretreatment, we sanded the metal with sanding paper on a block of wood, first vertically then horizontally. In the phosphoric acid pretreatment, we wiped the surface twice with phosphoric acid soaked paper, let it sit for approximately one minute, then neutralized by wiping the surface with a saturated baking soda solution. Then we wiped the metal twice with damp paper and dried it off with clean paper. The vinegar pretreatment was similar except that we used vinegar in place of phosphoric acid. For the soap pretreatment, we wiped the metal twice with soap-and-water-soaked paper then twice with damp paper and then dried it off with clean paper. We also attempted several tests in which we sanded first and then applied another pretreatment. For general applications of this methodology in Nicaragua, reusable cloths could be used in place of paper.
Next we painted all the pretreated areas and allowed the paint to dry for several days. Using a sharp knife, we scribed 5 8x8 (1 ~3 mm cell) grids into each pretreated area. Thus, each grid had 64 one square millimeter squares of paint that were not attached to each other. After that, we used the stickiest tape we could find (duct tape), adhered it to each grid, and then ripped it off. We counted the number of squares removed from each grid in that fashion and then performed statistical analysis on the resulting data.

...